A blasted surface that compares favourably with the ISO 8501-1 reference photographs can still be unfit to coat. Soluble salts, and chlorides in particular, are colourless, sit well below the resolution of the eye, and are not reliably removed by dry abrasive alone. Where they remain, the primer is applied over a hygroscopic layer that draws moisture through the film and drives osmotic blistering, blister populations that appear within months rather than years, and premature breakdown long before the coating's design life has elapsed.
For contractors working on coastal defences, ports, marine structures, highway assets and urban fabric exposed to winter de-icing salt, chloride testing is not a refinement to be added if the client asks. It is part of demonstrating that the substrate is what the specification assumed it to be.
Why a clean-looking surface proves very little
Visual standards assess preparation grade: freedom from rust, mill scale and previous coating. They say nothing about chemistry. Blasting will remove the bulk of a contaminated layer, but it also opens pits and creates a fresh micro-profile into which salt-laden moisture migrates. Weld toes, crevices, pitted areas and the underside of horizontal members are classic hold-up points. On a site half a mile inland, atmospheric chloride may be modest; on a quayside, a sea wall or a structure beside a treated carriageway, it can be substantial and highly variable across a single elevation.
The practical consequence is that a single reading from a convenient flat plate is not a dataset. Contamination is patchy, and the sampling plan has to reflect that.
Two instruments, one purpose
UK practice generally settles on one of two routes, and both end in a figure the coating manufacturer can accept or reject.
The Bresle patch method. A controlled volume of deionised water is injected into a flexible patch sealed to the surface, worked against the substrate for a defined period, then extracted. The extract is then measured for conductivity. The patch method is well established, documented in ISO 8502-6, and is the reference technique most coating inspectors will expect to see. Its quality depends heavily on technique: patch adhesion, the number of injection and extraction cycles, the dwell time, and cleanliness of the syringe all influence the result.
Direct conductivity measurement. Handheld instruments and field test kits give a conductivity reading from the extract, converted to surface density in milligrams per square metre using the standard relationship set out in ISO 8502-9. Temperature compensation matters; a reading taken in a cold January compound and one taken in a warm drying tent are not directly comparable unless the instrument corrects for it.
Some contractors use chloride-specific test strips for rapid screening. They are useful for triage and for confirming a trend across a large elevation, but they should not be offered as the sole evidence where the specification calls for a measured value. Screening tells you where to test properly; it does not replace the test.
Agreeing thresholds before mobilisation
Acceptance criteria belong in the coating specification, not in a conversation on the day. Ask the manufacturer in writing what surface salt density they will accept for the proposed system, and confirm whether the figure is expressed as chloride or as total soluble salts, since the two are not interchangeable. Typical project criteria for high-durability and immersion service sit well below the figures used for moderate atmospheric exposure, and marine schemes frequently adopt a stricter line again.
Where the manufacturer has no stated position, the specialist coating inspector or the client's technical authority should set the criterion. The important point is that the number is fixed before the first square metre is blasted, and that it is the same number in the method statement, the inspection and test plan and the handover pack.
Sampling frequency, location and timing
A workable regime for a mobile UK site usually combines area-based sampling with targeted sampling.
- Area-based: one test per agreed area, commonly in the order of one per 100 to 150 square metres of prepared steel, or one per structural member on fabricated work.
- Targeted: weld toes, pitted regions, horizontal surfaces, splash zones, the lower 500mm of a marine elevation, and any area where earlier readings were borderline.
- Timing: test after blasting and after any washing or reblast, immediately before priming. A surface that passes in the morning and sits through a damp afternoon has not been tested at the point of coating.
Record the location precisely enough that another party could return to the same square metre — member reference, elevation, grid line and a photograph with a scale.
What the record should contain
A defensible result is more than a number. Each entry should carry the date and time, the ambient and steel temperature, the method used, the patch or kit batch, the instrument identification and its calibration status, the operator, the extract volume and the result in milligrams per square metre alongside any strip or screening outcome. Results should be logged on the same sheet as the profile and cleanliness records so the three sit together at handover.
When a reading fails
The first response should be diagnosis, not primer. Confirm the instrument is functioning and in calibration, repeat the test at the same location and at a nearby control point, and check whether the failure is isolated or a pattern across the elevation.
Where contamination is genuine, the practical remedies are reblasting, or washing with clean water at controlled pressure followed by drying and retesting, or both. Washing with contaminated water, or with water of unknown quality, will simply redistribute the problem and can leave a residue of its own. Retest after every intervention, and record the retest as a separate result rather than overwriting the original. Priming over a failed reading converts a solvable preparation issue into a coating defect with a warranty attached to it.
The economics are straightforward. A chloride test takes minutes. Removing a prematurely failed coating system from a marine structure takes a scaffold, a blast crew and a second programme.